382 Engineering of Polymers and Chemical Complexity
method at 8000 rpm continued for 10 min, dried at 60 0C for a time period of
3 h and which was used again for loading of PAA layer.
(3) Deposition of PAA Polyelectrolyte Layer on Benzotriazole Loaded PANI
Encapsulated Zn2PMoO7 Nanoparticles: PAA polyelectrolyte layer was
adsorbed on benzotriazole loaded PANI encapsulated ZMPnanoparticles to
attain sustained and responsive release of corrosion inhibitor at varying pH
environment and to make ZMP nanocontainer suitable to prepare alkyd resin
based paint formulation. For the adsorption of PAA layer, 2 mg ml-1 of con-
centration solution of PAA was prepared in 0.1 N NaCl solution by using of
sonochemical irradiation for time duration of 20 min. ...